What GH4169 (UNS N07718) High-Temperature Alloy Is
The alloy known internationally as UNS N07718 and in the Chinese system as GH4169 is a precipitation-hardening nickel-based superalloy built for service from cryogenic temperatures up to about 700 degrees Celsius. Below roughly 650 degrees Celsius its yield strength is among the highest of any wrought superalloy, which explains its position in aircraft engines, rocket propulsion hardware, nuclear components and sour-service oilfield equipment.
The material combines high strength with fatigue resistance, oxidation resistance, radiation tolerance and long-term structural stability, and it can be forged, rolled and machined into complex shapes. A second defining characteristic is metallurgical sensitivity: the balance between the strengthening precipitates and the grain-boundary phases depends strongly on hot-working and heat-treatment practice, so the same chemistry can deliver very different property levels depending on how it is processed.
Chemical Composition and Physical Constants
Composition is controlled to a narrow window because niobium, titanium and aluminium drive the precipitation response. Typical limits are shown below; the controlling document is the specification named on the order, such as ASTM B637 for bars and forgings.
| Element | Typical Range, % | Function |
|---|---|---|
| Nickel | 50 - 55 | Austenitic matrix, corrosion and oxidation resistance |
| Chromium | 17 - 21 | Oxidation and hot-corrosion resistance |
| Iron | Remainder (balance) | Matrix, cost control |
| Niobium plus tantalum | 4.75 - 5.50 | Forms the principal strengthening phase |
| Molybdenum | 2.80 - 3.30 | Solid-solution strengthening, pitting resistance |
| Titanium | 0.65 - 1.15 | Age-hardening addition |
| Aluminium | 0.20 - 0.80 | Age-hardening addition |
| Carbon | 0.08 maximum | Controlled to limit carbide networks |
| Cobalt | 1.00 maximum | Residual |
| Boron | 0.006 maximum | Grain-boundary control |
Physical constants used in design calculations include a density of about 8.2 grams per cubic centimetre and a melting range of approximately 1260 to 1340 degrees Celsius. The austenitic face-centred-cubic structure is stable across the working range, which is why the alloy retains useful toughness without a ductile-to-brittle transition.
Mechanical Properties and Temperature Capability
In the solution-treated condition the alloy already offers high strength, and the aged condition raises it further. Minimum room-temperature values widely specified for solution-treated material are a tensile strength of 965 MPa, a 0.2 percent proof strength of 550 MPa and an elongation of 30 percent, with a Brinell hardness not exceeding 363 HB. Aged material is normally specified to higher strength levels agreed between buyer and supplier.
Cryogenic service: stable properties and good toughness down to about minus 253 degrees Celsius, used in liquid hydrogen and other cryogenic systems.
Elevated service: useful to about 700 degrees Celsius with good creep and stress-rupture strength, and excellent fatigue strength under cyclic loading.
Oxidation: a protective chromium-rich oxide scale gives good resistance in air at 1000 degrees Celsius for short-term exposure.
Corrosion: resistant to stress corrosion cracking and pitting in many aqueous and sour environments; resistance is reduced by highly oxidising or strongly reducing media.
The strengthening phase is a body-centred-tetragonal nickel-niobium precipitate that forms during ageing, while a niobium-rich grain-boundary phase formed during controlled heat treatment improves notch ductility. Because the alloy is slow-hardening, it can be welded in the annealed condition and aged afterwards without cracking.
Hot Working, Cold Working and Welding
Hot working of this alloy requires discipline. The recommended working range is about 1120 down to 900 degrees Celsius, with the charge heated to the upper part of the range for the first passes. Deformation should not be continued below 960 degrees Celsius; final passes at lower temperature produce a partially recrystallised structure with poor creep resistance. Water quenching or another rapid cooling method should follow, and timely annealing prevents undesirable phase precipitation in the as-worked structure.
Cold forming is carried out after solution treatment. The alloy work-hardens faster than austenitic stainless steel, so press capacity, tool radii and pass schedules must be adjusted, and intermediate annealing is planned into multi-stage operations. Welding performance is generally good: gas tungsten arc welding, electron beam welding, seam welding and resistance spot welding are all used in production, with clean joint preparation, matched or matching filler metal and adequate shielding to prevent niobium and titanium loss.
Heat Treatment Practice
Two routes dominate. Aerospace parts normally receive the standard solution treatment followed by a two-step age, while less demanding parts may be direct-aged from the hot-worked condition. A typical two-step age holds the part at about 720 degrees Celsius for eight hours, cools it at a controlled rate of roughly 50 degrees Celsius per hour to about 620 degrees Celsius, holds for a further eight hours, and finishes with an air cool. Solution treatment is carried out near 950 to 980 degrees Celsius depending on the product form and the required grain size.
Deviation from the specified cycle changes the precipitate size and therefore the balance of strength, ductility and rupture life, which is why furnace records, thermocouple placement and load thermocouples are inspected during qualification.
Frequently Asked Questions
Q: What is the Chinese equivalent of UNS N07718?
The Chinese designation is GH4169, produced to the corresponding national specification. Equivalent designations elsewhere include W.Nr. 2.4668 and NA 51.
Q: Can GH4169 be used above 700 degrees Celsius?
Strength falls quickly above about 700 degrees Celsius, and long exposure causes precipitate coarsening. Other nickel-based grades are usually selected for sustained service above that temperature.
Q: Why must hot working stop above 960 degrees Celsius?
Finishing below that temperature leaves unrecrystallised grains and a harmful phase distribution that reduces stress-rupture life even if short-term tensile properties still pass.
Q: Is the alloy weldable in the aged condition?
Welding is normally performed in the solution-treated or annealed condition. Welding aged material risks strain-age cracking in the heat-affected zone, so ageing is carried out after welding.
Q: What causes the alloy to be difficult to machine?
High temperature strength, rapid work hardening and poor thermal conductivity concentrate heat at the cutting edge, so rigid setups, sharp positive geometry and generous coolant flow are essential.
Q: Which product forms are commonly supplied?
Round bar, wire, strip, sheet, seamless tube, valve seats, balls, flanges and forgings are standard, with the governing specification chosen for the form, for example ASTM B637 for bars and forgings.