The Metallurgical Family Difference
The two grades belong to different alloy families, and that is the origin of every practical difference between them. UNS N06600 is a nickel-chromium-iron alloy with a nickel content of 72.0 percent minimum and a chromium range of 14.0 to 17.0 percent; the balance is iron at 6.0 to 10.0 percent. UNS N08800 is a nickel-iron-chromium alloy in which iron is the largest single element by specification at 39.5 percent minimum, with 30.0 to 35.0 percent nickel and 19.0 to 23.0 percent chromium. One is a nickel alloy with iron as an addition; the other is an iron-based alloy with enough nickel and chromium to remain fully austenitic.
| Element (wt %) | UNS N06600 (ASTM B166 / B167) | UNS N08800 (ASTM B408 / B407) |
|---|---|---|
| Nickel | 72.0 min | 30.0-35.0 |
| Chromium | 14.0-17.0 | 19.0-23.0 |
| Iron | 6.0-10.0 | 39.5 min |
| Carbon | 0.15 max | 0.10 max |
| Aluminium | Not specified | 0.15-0.60 |
| Titanium | Not specified | 0.15-0.60 |
| Copper | 0.50 max | 0.75 max |
The higher chromium of N08800 gives it better resistance to oxidation and to sulphur-bearing atmospheres at temperature. The much higher nickel of N06600 gives it resistance to chloride stress corrosion cracking and to caustic environments that the iron-based grade cannot match.
High-Temperature Behaviour
Both grades are used in furnaces, but for different reasons. N08800 is structurally stable in long-term service to about 1100 °C because its austenitic matrix resists the sigma-phase and embrittlement problems that affect some iron-based alloys, and its chromium content supports a protective scale. For creep-limited duty above about 700 °C the higher-carbon variants are used instead: UNS N08810, with carbon specified at 0.05 to 0.10 percent, and UNS N08811, with carbon at 0.06 to 0.10 percent and a combined aluminium plus titanium range of 0.85 to 1.20 percent. The carbon level and the carbide-forming additions are what raise stress-rupture strength; a standard N08800 tube should not be substituted for an N08810 or N08811 tube in a creep-limited design.
N06600 tolerates continuous exposure to roughly 1095 °C in oxidising atmospheres with modest load, and it holds up well under repeated thermal cycling, which is why it is common in heat treating fixtures, radiant tubes and thermocouple sheaths. Its weaker point is high-temperature strength: annealed N06600 bar is specified under ASTM B166 at a minimum tensile strength of 550 MPa and a minimum yield strength of 240 MPa, which is a lower strength baseline than designers sometimes assume from the alloy name.
Corrosion Performance
In chloride-bearing water the ranking is clear. N06600 is effectively immune to chloride stress corrosion cracking at practical stress levels and is widely used in caustic evaporators because it also resists caustic cracking. N08800 offers better resistance than austenitic stainless steels but is not in the same class as a high-nickel alloy, and it can suffer stress corrosion cracking in hot concentrated chlorides or in polythionic acid conditions. Where the medium is high-temperature water or steam with chloride contamination, that difference decides the material.
Against oxidising high-temperature atmospheres the ranking reverses. The 19.0 to 23.0 percent chromium of N08800, combined with its aluminium and titanium additions, produces a more protective and more adherent scale than N06600 does, so N08800 is frequently the better choice for furnace internals exposed to sulphur-bearing flue gas, provided the temperature is held below the point at which nickel sulphide formation becomes a risk.
Cost, Availability and Fabrication
N08800 contains less than half the nickel of N06600, so its raw material cost is materially lower and its price is less exposed to nickel market movement. Both grades are produced as seamless tube and pipe, with ASTM B163 and B407 covering N08800 in tube and pipe forms and ASTM B167 covering N06600, and both are available as bar under ASTM B408 and B166 respectively. Both are welded by gas tungsten arc with matching filler metal. N06600 is generally more forgiving in welding because its higher nickel content reduces the risk of solidification cracking and it does not require the carbide-stabilising heat treatment that the higher-carbon furnace grades need.
Making the Selection
Choose N06600 where chloride or caustic corrosion resistance governs, where components are thermally cycled, or where a moderate load is carried at high temperature. Choose N08800 where oxidation and scaling resistance in a furnace atmosphere governs, where cost and nickel price exposure matter, or where a creep-limited design can be met by specifying the higher-carbon N08810 or N08811 variant. Where both environments appear in the same system, the correct answer is usually a joint that places each alloy where its strength applies.
Frequently Asked Questions
Q: Is Inconel 600 better than Incoloy 800?
A: Neither is universally better. N06600 is superior in chloride and caustic service and in thermal cycling; N08800 is superior in oxidising and sulphur-bearing furnace atmospheres and costs less.
Q: Are these two alloys the same family?
A: No. N06600 is a nickel-chromium-iron alloy with 72.0 percent minimum nickel, while N08800 is a nickel-iron-chromium alloy with iron at 39.5 percent minimum and nickel at 30.0 to 35.0 percent.
Q: Can Incoloy 800 be used for creep-limited service at 800 degrees C?
A: Only by specifying the higher-carbon variants. UNS N08810 and UNS N08811 are the grades intended for creep-limited duty, not standard UNS N08800.
Q: Which grade resists chloride stress corrosion cracking better?
A: N06600, because of its higher nickel content. N08800 resists cracking better than austenitic stainless steel but is not equivalent to a high-nickel alloy.
Q: Which grade is cheaper?
A: N08800, because it contains less nickel. Its price is also less sensitive to nickel market movement, which matters for long-lead projects.
Q: What specifications cover the tube and bar forms?
A: ASTM B163 and B407 for N08800 tube and pipe, ASTM B408 for N08800 bar, and ASTM B167 and B166 for the equivalent N06600 product forms.