May 16, 2025 Leave a message

Datasheet-For-Inconel-600-1-7-(1)-1-6.pdf

Heat Treatment System for UNS N06600 Plate: Annealing and Stress Relief

Why Heat Treatment Decides UNS N06600 Performance

UNS N06600 is a nickel-chromium-iron alloy with a fully austenitic, single-phase structure. There is no martensite in this material at any normal condition, and no phase ratio has to be balanced by heat treatment: the austenitic matrix is produced by the alloy chemistry itself. What the heat treatment cycle does control is grain size, residual stress, and the amount of chromium carbide left on the grain boundaries, and those three factors decide whether a plate performs in high temperature or corrosive service.

Plate for pressure and high temperature duty is normally ordered in the annealed condition to ASTM B168, with the corresponding ASME SB-168 designation for pressure vessel application. Sheet, strip and plate are also covered by AMS 5540 and bar and forging stock by AMS 5665 where aerospace release is required. Those specifications, not a general workshop rule, govern the temperature, holding time and cooling rate that must be recorded on the material certificate.

Chemistry and Mechanical Requirements of the Plate

Element, % Limit (ASTM B168, UNS N06600)
Nickel (Ni) 72.0 min
Chromium (Cr) 14.0 - 17.0
Iron (Fe) 6.0 - 10.0
Carbon (C) 0.15 max
Manganese (Mn) 1.00 max
Silicon (Si) 0.50 max
Copper (Cu) 0.50 max
Sulphur (S) 0.015 max

Annealed plate, tensile strength: 550 MPa (80 ksi) minimum.

Annealed plate, yield strength at 0.2% offset: 240 MPa (35 ksi) minimum.

Annealed plate, elongation in 50 mm: 30% minimum.

Hardness is normally reported for information and follows the annealed condition of supply.

The high nickel content stabilises the austenitic structure, the chromium content provides the protective oxide needed for high temperature service, and the controlled carbon range allows useful strength to be retained at temperature. Users should not treat the 0.15% carbon maximum as a target: low carbon heats are selected when the plate will be welded and exposed to sensitising temperatures.

Solution Annealing and Quenching

The purpose of solution annealing is to dissolve carbides that formed during hot rolling or prior service and to recrystallise the worked structure, producing a uniform austenitic grain structure with the carbon held in solution. The plate is heated uniformly through the section, held at temperature, and then cooled rapidly enough to prevent carbides from re-forming on the grain boundaries during the passage through the sensitising range.

Stage Typical practice Purpose
Charging Charge below 400 °C in a clean, sulphur-free furnace atmosphere Avoids thermal shock and contamination of the surface
Annealing hold 1040 - 1140 °C (1900 - 2085 °F), typically 1 hour per 25 mm of thickness Dissolves carbides and recrystallises the structure
Cooling Water quench preferred; rapid forced air for thin plate Keeps carbon in solution and limits grain-boundary carbide precipitation
Post-treatment cleaning Pickling or abrasive blasting to remove oxide scale Restores a clean surface for corrosion service and inspection

Time at temperature matters more than the exact point within the range, but excessive hold at the top of the range coarsens the grains and lowers room temperature strength. A fully recrystallised, fine grain structure is normally specified for corrosive service, while somewhat coarser grains are accepted for high temperature creep duty because fewer grain boundaries slow diffusion-controlled deformation. Charging plate into a hot furnace is bad practice: it produces non-uniform grain growth and distortion across the section.

Quenching must follow without delay once the hold is complete. Slow cooling through the 425 to 760 °C range allows chromium-rich carbides to precipitate at the grain boundaries and depletes the adjacent matrix of chromium, which is the classic sensitisation mechanism. In mildly corrosive service the effect may be invisible, but in chloride or acidic environments the sensitised boundaries become preferential paths for intergranular attack and eventual component failure.

Stress Relief and Carbide Precipitation Control

Fabrication introduces residual stress from forming, machining and welding. Stress relief treatments are applied to reduce that stress before the part enters service, or between forming stages, and their temperature has to be chosen with care because the beneficial range overlaps the carbide precipitation range.

Low temperature stress relief: Applied below the precipitation range for dimensional stability and relief of forming stress, with minimal effect on corrosion resistance.

Intermediate temperature relief: Effective for relieving welding stress, but it sits within the sensitising range, so it is normally limited to service where intergranular corrosion is not the governing risk, or it is followed by a full solution anneal.

Full solution anneal after fabrication: The preferred route for plate that will face chlorides, acids or high purity process streams, since it dissolves any carbides and restores the boundary chemistry in one step.

Welded assemblies: A post-weld solution anneal is specified for severe service. Where the assembly cannot be re-annealed, low carbon heats should be used and the actual thermal history recorded.

Furnace atmosphere is part of the treatment. Sulphur-bearing fuels and reducing atmospheres can attack the alloy surface and change its chemistry, so clean, controlled atmosphere furnaces are used for final anneals. Temperature uniformity across the furnace, verified with a survey before production runs, determines whether the plate at the edge of the load receives the same treatment as the plate in the centre.

Inspection, Grain Size and Test Methods

Grain size: Measured on a polished and etched section, normally reported against one of the standard grain size comparison methods, and quoted together with the test location.

Tensile and hardness testing: The room temperature tensile properties listed above are verified per heat treatment lot, with test specimens taken in the direction required by the plate standard.

Intergranular corrosion testing: The accepted method for nickel-rich chromium-bearing alloys is the ferric sulphate plus sulphuric acid boiling test, used to confirm that the annealed plate has not been sensitised by the delivered heat treatment.

Corrosion rate checks in specific media: Where the plant medium is known, coupons are exposed to that medium and the mass loss reported as a penetration rate so the designer can compare it with the allowable allowance.

Certification: Temperature, holding time, cooling method, furnace identification and test results are recorded on the material certificate so the heat treatment system can be audited later.

Frequently Asked Questions

Q: Does UNS N06600 contain martensite?
No. The alloy is fully austenitic at all normal service and heat treatment conditions, because the high nickel content stabilises the austenitic matrix. Statements describing an austenite to martensite ratio in this grade are incorrect.

Q: Why is a fast quench necessary after annealing?
Rapid cooling keeps carbon in solution instead of allowing chromium-rich carbides to precipitate at the grain boundaries. Slow cooling through the intermediate temperature range causes sensitisation and reduces resistance to intergranular attack.

Q: Can stress relief be applied instead of a full anneal?
Stress relief reduces residual stress but does not remove carbides already present at the grain boundaries. Where corrosion resistance governs the design, a full solution anneal is the correct treatment.

Q: What grain size is normally specified?
The plate standard, together with the application, fixes the requirement. Corrosion service usually calls for a fine, uniform recrystallised grain structure, while creep-limited high temperature service tolerates a coarser structure.

Q: Which test confirms that the plate is not sensitised?
The ferric sulphate plus sulphuric acid boiling test applied to nickel-rich chromium-bearing alloys is the standard method for detecting susceptibility to intergranular corrosion, and it is commonly specified as a mill supplementary requirement.

Q: How should heat treated plate be handled afterwards?
Pickle or blast it to remove scale, keep it free of carbon steel contact, oil, marking inks and chloride-bearing dust, and store it clear of the ground on clean timber or polymer supports until fabrication begins.