Grade 3 titanium is a commercially pure titanium grade (UNS R50550) that sits between Grade 2 and Grade 4 in the ASTM classification. Because it carries a higher oxygen content than Grade 2, it delivers roughly 30 percent more yield strength while keeping the ductility and corrosion resistance that make unalloyed titanium attractive in chemical, medical and marine service. This guide covers the annealed yield strength of Grade 3 titanium, the effect of cold working, its density and hardness limits, and the standards that govern supply.
What Is the Yield Strength of Grade 3 Titanium?
In the annealed condition, which is the state in which commercial purity titanium is normally supplied and used, Grade 3 titanium has a yield strength (0.2 percent offset) of 380-480 MPa (55,000-70,000 psi). ASTM B265, the specification for titanium and titanium alloy strip, sheet and plate, fixes a minimum yield strength of 380 MPa for annealed Grade 3 so that every conforming lot behaves predictably in a stressed or pressure-retaining application.
The same specification sets a minimum tensile strength of 450 MPa and a minimum elongation of 18 percent in 50 mm for annealed Grade 3. That combination is why designers treat it as the medium-strength commercial purity grade: clearly stronger than Grade 1 or Grade 2, yet still more formable and weldable than Grade 4.
| Standard | Product form | Min. yield strength | Min. tensile strength | Min. elongation |
|---|---|---|---|---|
| ASTM B265 | Strip, sheet, plate | 380 MPa | 450 MPa | 18 % |
| ASTM B348 | Bar, billet, forging stock | 380 MPa | 450 MPa | 18 % |
| ASTM F67 | Wrought implant stock | 380 MPa | 450 MPa | 18 % |
| ISO 5832-1 | Wrought implant stock | 380 MPa | 450 MPa | 18 % |
How Cold Working Changes the Yield Strength
Cold rolling, drawing or stretch forming raises the yield strength of Grade 3 titanium by approximately 10-20 percent through work hardening, taking typical values to roughly 420-550 MPa (up to about 80,000 psi). Ductility falls in step, so cold-worked stock is normally chosen where stiffness, spring behaviour or fatigue strength matters rather than where severe forming is still required. When further shaping is needed, a vacuum or inert-atmosphere anneal restores the equilibrium structure and returns the material close to its 380-480 MPa band.
Annealed strip and plate: 380-480 MPa yield, maximum formability.
Cold rolled 10-20 percent: roughly 420-550 MPa yield, moderate ductility.
Stress relief after forming: typically 1 hour at 540-650 °C in vacuum or high-purity argon.
Chemical Composition of Grade 3 Titanium
Grade 3 is unalloyed titanium; its strength comes from tightly controlled interstitial elements rather than from alloying additions. Typical maximum values by weight are:
Titanium: balance
Oxygen: 0.35 % max - the main strengthening element
Nitrogen: 0.05 % max
Carbon: 0.10 % max
Iron: 0.30 % max
Hydrogen: 0.015 % max
Because oxygen is the dominant strengthener, a supplier that holds oxygen at the low end of the range will produce material closer to 380 MPa, while mid-range oxygen produces values nearer 450-480 MPa. Buyers who need tight property windows should therefore state the intended oxygen target on the purchase order in addition to the ASTM chemistry limits.
Density and Physical Properties
Density is essentially the same across the commercial purity grades: 4.51 g/cm³ (0.163 lb/in³) at room temperature. That is about 60 percent of the 7.85 g/cm³ of carbon steel and 56 percent of the 8.96 g/cm³ of copper, which is the main reason Grade 3 is selected where weight reduction matters but full alloy strength is unnecessary.
| Property | Value |
|---|---|
| Density | 4.51 g/cm³ (0.163 lb/in³) |
| Modulus of elasticity | approx. 103 GPa (14.9 Msi) |
| Thermal conductivity at 20 °C | approx. 21.9 W/m·K |
| Melting point | approx. 1668 °C |
| Coefficient of thermal expansion | approx. 8.6 µm/m·K (20-100 °C) |
Hardness Range of Grade 3 Titanium
Hardness depends on the processing state and on the test method used, so a single figure is misleading. The ranges below reflect normal commercial product tested with standard loads.
| Condition | Brinell (3000 kg / 10 mm) | Rockwell | Vickers |
|---|---|---|---|
| Annealed | 150-180 HB | B80-B90 HRB | 160-200 HV |
| Cold worked 20-30 % | 180-220 HB | B90-B95 HRB | 200-240 HV |
Even in the harder cold-worked state, Grade 3 remains machinable and weldable, which distinguishes it from higher-strength alloyed grades where preheat, post-weld heat treatment and dedicated tooling become mandatory.
Frequently Asked Questions
Q: What is the minimum yield strength of Grade 3 titanium?
380 MPa (55,000 psi) in the annealed condition, as specified in ASTM B265 for strip, sheet and plate and in ASTM B348 for bar and billet.
Q: Is Grade 3 titanium stronger than Grade 2?
Yes. Annealed Grade 2 has a minimum yield strength of about 275 MPa, while Grade 3 is specified at a 380 MPa minimum, so Grade 3 is roughly 30 to 40 percent stronger.
Q: What is the density of Grade 3 titanium?
4.51 g/cm³, or 0.163 lb/in³, which is about 60 percent of the density of steel and 56 percent of that of copper.
Q: Can the yield strength be increased by cold working?
Yes. Cold rolling or drawing typically lifts yield strength by 10-20 percent to about 420-550 MPa, with a corresponding loss of elongation.
Q: What hardness does Grade 3 titanium have?
Annealed material normally falls in the 150-180 HB, 160-200 HV or B80-B90 HRB range; cold-worked material is harder at roughly 180-220 HB.
Q: Which standards cover Grade 3 titanium?
ASTM B265 for plate, sheet and strip, ASTM B348 for bar and billet, ASTM F67 and ISO 5832-1 for wrought implant material.