Material Overview
Alloy X-750 (UNS N07750) is a nickel-chromium material made precipitation hardenable by the addition of aluminium and titanium. It offers good corrosion and oxidation resistance together with high tensile and creep-rupture properties at temperatures up to about 1300 °F (700 °C). Because it resists relaxation so well, it is widely used for high-temperature springs and bolts, and it also appears in gas turbines, rocket engines, nuclear reactors, pressure vessels, tooling and aircraft structures.
The alloy is normally supplied as bar, wire, forging stock, plate, sheet and strip, and as seamless or welded tube. Properties depend strongly on the heat treatment condition, so the material certificate should always be read together with the treatment cycle that produced it.
Chemical Composition Limits
Weight percent limits for the standard wrought grade:
| Element | Nickel plus cobalt | Chromium | Iron | Titanium | Aluminium | Niobium plus tantalum | Manganese | Silicon | Sulfur | Copper | Carbon | Cobalt |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Content, wt % | 70.0 min | 14.0 - 17.0 | 5.0 - 9.0 | 2.25 - 2.75 | 0.40 - 1.00 | 0.70 - 1.20 | 1.00 max | 0.50 max | 0.010 max | 0.50 max | 0.08 max | 1.00 max |
A modified melting variant for forging stock, designated UNS N07752, is available in billets and applies a maximum of 0.05% to both carbon and cobalt. That lower interstitial and cobalt level is chosen where nuclear or fatigue-sensitive forgings must meet tighter cleanliness and activation limits, and it must be requested explicitly because it is not interchangeable with the standard grade on the certificate.
Typical Mechanical Properties
Room-temperature values for bar stock in the precipitation hardened condition:
| Product and size | Tensile strength | Yield strength, 0.2% offset | Elongation in 4D | Reduction of area |
|---|---|---|---|---|
| Bar under 4.0 in | 165.0 ksi (approx. 1140 MPa) | 105 ksi (approx. 725 MPa) | 20% | 25% |
| Bar 4.0 in and over | 160 ksi (approx. 1100 MPa) | 100 ksi (approx. 690 MPa) | 15% | 17% |
Larger sections show slightly lower strength because cooling rate and the amount of deformation through the section both change. The values above follow the requirements of AMS 5667, which specifies that material processed to the 1625 °F solution treatment with air cooling, followed by the equalising and precipitation treatments, meets these minimum room-temperature properties. Hardness for material in that condition normally falls in the range 302 to 363 BHN, and hardness testing is often used as a quick acceptance check on finished parts.
Heat Treatment and Condition
Solution treatment: the material is soaked and air cooled to dissolve the strengthening elements before forming.
Equalising and ageing: the two-stage treatment specified in the applicable AMS or ASTM document develops the final strength and stress-rupture properties.
Condition of supply: bar is usually supplied solution treated and aged to the specified cycle, while wire for springs is supplied in a condition suited to coiling before ageing.
Verification: because hardness alone cannot separate all conditions, tensile testing on a per-heat or per-lot basis is included for critical applications.
Design and Fabrication Notes
The alloy work hardens quickly, so forming operations should be planned with generous radii and, where possible, carried out before ageing. Machining in the aged condition gives a good surface finish with carbide tooling and reduced cutting speeds. Welding is performed with matching filler metal and is usually followed by the specified ageing treatment so that the joint recovers its strength. At high temperature a protective oxide forms on the surface and slows further degradation, which supports the use of the material in combustion and air atmospheres; however, the alloy is not intended to replace molybdenum-bearing grades in severe wet chloride service.
Typical Uses
High-temperature springs, bolts and fasteners; turbine blades, wheels and seals; rocket engine components; nuclear reactor internals and springs; pressure vessel internals; hot forming tools and dies; and aircraft structural parts that must retain stiffness and strength at temperature.
Frequently Asked Questions
Q: What is the difference between UNS N07750 and UNS N07752?
N07752 is the forging billet variant with carbon and cobalt each limited to 0.05% maximum. It is selected for tighter cleanliness and reduced activation requirements and is not freely interchangeable with the standard grade.
Q: Which treatment produces the properties quoted in the data sheet?
The figures follow AMS 5667, based on a 1625 °F solution treatment with air cooling and then the equalising and precipitation treatments defined in that specification.
Q: Why is hardness quoted as a range rather than a single value?
Because hardness responds to section size, cooling rate and the exact ageing cycle. The 302 to 363 BHN range corresponds to the specified treated condition and is used as an acceptance check, not as a substitute for tensile testing.
Q: How should the material be ordered?
State the grade and UNS number, the product form and size, the heat treatment condition and the governing AMS or ASTM specification; where a forging billet variant is needed, name it explicitly.
Q: Can the alloy be welded and then left in the as-welded condition?
It can be welded, but the weld zone loses strength relative to the aged base metal, so the specified post-weld ageing treatment is normally applied to restore properties.
Q: What is supplied as quality documentation?
An EN 10204 3.1 mill certificate showing heat number, chemical analysis, heat treatment record and mechanical test results, together with dimensional and non-destructive inspection records where specified.