1.1 Solution Annealing (Solution Heat Treatment)
Purpose:
To dissolve any segregations, carbides, or other microstructural inhomogeneities formed during manufacturing.
To achieve a uniform, fine-grained microstructure.
To optimize corrosion resistance and ductility.
Typical Temperature:
1100–1200°C (2010–2190°F)
Holding Time:
30–60 minutes (depending on thickness; thicker sections require longer times).
Cooling Method:
Water quenching or rapid air cooling to retain the homogeneous solid-solution structure and prevent excessive grain growth during slow cooling.
Applications:
After hot working (forging, extrusion, rolling) to restore ductility.
To improve corrosion resistance in critical applications.
To prepare the material for subsequent welding or machining.
1.2 Stress Relief Annealing (Stress Relief Heat Treatment)
Purpose:
To reduce residual stresses from welding, machining, or forming.
To minimize the risk of stress corrosion cracking (SCC), especially in caustic or chloride environments.
To improve dimensional stability.
Typical Temperature:
700–900°C (1290–1650°F)
Holding Time:
1–4 hours (based on thickness and residual stress level).
Cooling Method:
Air cooling or furnace cooling (slow cooling is acceptable here, as the goal is stress relaxation, not microstructure refinement).
Applications:
After welding thick sections or highly restrained joints.
For components in high-temperature caustic service (e.g., NaOH evaporators).
To reduce distortion during machining.
1.3 Annealing for Improved Machinability
Purpose:
To soften the material and improve machinability.
To reduce work hardening from previous cold working.
Typical Temperature:
870–980°C (1600–1800°F)
Holding Time:
30–60 minutes
Cooling Method:
Air cooling
Note:
This is not a standard "named" heat treatment but is often used in practice to prepare Inconel 600 for machining operations.
1.4 Cold Work Recovery Annealing
Purpose:
To recover ductility and reduce hardness after cold working (e.g., cold rolling, drawing).
To eliminate residual stresses from cold forming.
Typical Temperature:
800–900°C (1470–1650°F)
Holding Time:
30–120 minutes
Cooling Method:
Air cooling
Effect:
Restores ductility while maintaining reasonable strength.
Prevents embrittlement during subsequent high-temperature service.
1.5 Post-Weld Heat Treatment (PWHT)
Purpose:
To relieve welding residual stresses.
To reduce the risk of SCC in aggressive environments.
To improve toughness in the weld and heat-affected zone (HAZ).
Typical Temperature:
700–900°C (1290–1650°F)
Holding Time:
1–4 hours
Cooling Method:
Air cooling or slow furnace cooling
Note:
PWHT is not always required for Inconel 600, but is often specified for thick sections or corrosive service conditions.




1.6 Grain Growth Control Heat Treatment
Purpose:
To adjust grain size for specific applications (e.g., fine grains for fatigue resistance, coarser grains for creep strength).
Typical Temperature:
950–1150°C (1740–2100°F)
Holding Time:
Short times (minutes to tens of minutes) to avoid excessive grain growth.
Cooling Method:
Rapid cooling to preserve the desired grain size.
Application:
In specialized high-temperature components where a specific grain size is required.
1.7 Summary of Key Heat Treatment Regimes for Inconel 600
Solution Annealing: 1100–1200°C, 30–60 min, water/air quench
Stress Relief: 700–900°C, 1–4 h, air/furnace cool
Machinability Annealing: 870–980°C, 30–60 min, air cool
Recovery Annealing (after cold work): 800–900°C, 30–120 min, air cool
Post-Weld Heat Treatment: 700–900°C, 1–4 h, air/furnace cool
Grain Size Control: 950–1150°C, short hold, rapid cool
Inconel 600's heat treatment is primarily focused on solution annealing for microstructure control and stress relief for corrosion and mechanical stability, rather than strength enhancement through precipitation hardening.