Two Grades, One Base Alloy
Monel 400 (UNS N04400, W.Nr. 2.4360) and Monel K500 (UNS N05500, W.Nr. 2.4375) both belong to the nickel-copper family, containing roughly two thirds nickel and one third copper. They behave similarly in seawater, in hydrofluoric acid and in alkaline chlorides, and both are essentially non-magnetic at room temperature. The difference is that K500 is a precipitation-hardenable modification of the 400 composition, and that single metallurgical change produces a completely different set of mechanical properties while leaving the corrosion behaviour almost untouched.
Chemical Composition Differences
The aluminium and titanium additions in K500 are the whole story, and the tighter impurity limits are there to protect the ageing response. Ranges below follow ASTM B164 for the 400 grade and ASTM B865 for K500.
| Element (wt. %) | Monel 400, UNS N04400 | Monel K500, UNS N05500 |
|---|---|---|
| Nickel | 63.0 - 70.0 | 63.0 - 70.0 |
| Copper | 28.0 - 34.0 | 27.0 - 33.0 |
| Aluminium | 0.50 max | 2.30 - 3.15 |
| Titanium | 0.35 max | 0.35 - 0.85 |
| Iron | 2.50 max | 2.00 max |
| Manganese | 2.00 max | 1.50 max |
| Carbon | 0.30 max | 0.25 max |
| Sulfur | 0.024 max | 0.010 max |
The 400 grade is a simple binary alloy that can be strengthened only by cold working. K500 carries deliberate additions of aluminium and titanium in the range that produces a controlled precipitation reaction during ageing.
Heat Treatment and Strengthening Mechanism
Monel 400 is normally supplied annealed or cold worked and requires no thermal hardening step, which makes it easy to weld and form after final heat treatment. Monel K500 is solution treated at approximately 980 C and quenched, then aged at about 595 C for roughly 16 hours to precipitate fine Ni3(Al, Ti) particles throughout the matrix. These precipitates obstruct dislocation movement and produce the strength and hardness that the 400 grade cannot reach. Because the precipitates coarsen if the material is overheated, any welding on K500 components has to be followed by a re-solution and ageing treatment if full base-metal properties are required in the joint.
Mechanical Properties Compared
Typical room-temperature values are shown below. The specification minima in ASTM B164 and ASTM B865 vary with product form and condition, so the applicable line of the specification should always be checked for the exact size and temper being purchased.
| Property at room temperature | Monel 400, annealed | Monel K500, aged |
|---|---|---|
| Tensile strength | About 550 MPa | About 1,100 MPa |
| Yield strength, 0.2 % offset | About 240 MPa | About 790 MPa |
| Elongation in 50 mm | About 30 - 40 % | About 20 % |
| Hardness | Typically 60 - 80 HRB | Typically 27 - 35 HRC |
| Modulus of elasticity | About 179 GPa | About 179 GPa |
The practical consequence is straightforward. K500 resists wear, galling, erosion and fatigue loading far better than the 400 grade, which is why pump shafts, impellers, valve stems, scraper blades, fastener stock and drill collars are made from K500. Where static strength is adequate and formability or weldability is more important, the 400 grade is cheaper and easier to process.
Corrosion Behaviour and Temperature Limits
Both grades resist flowing seawater, neutral and alkaline salt solutions, hydrofluoric acid and many organic acids, and both are resistant to chloride stress corrosion cracking. Differences appear in three areas. First, the higher hardness of K500 gives it markedly better resistance to erosion and impingement, which matters in pumps and agitators. Second, the alloying additions mean K500 is slightly less resistant than 400 in certain strongly reducing acid environments. Third, the ageing precipitates limit the service temperature: K500 is generally restricted to below about 480 C, while the 400 grade is used from cryogenic temperature up to roughly 480 C in pressure equipment with design allowables listed in the applicable ASME code.
Neither grade should be used with strongly oxidizing media such as nitric acid, nor with aerated acids containing oxidizing impurities, and both require attention to crevice geometry in stagnant seawater because deposits can promote localised attack.
Applicable Standards and Availability
| Product form | Monel 400 | Monel K500 |
|---|---|---|
| Plate, sheet, strip | ASTM B127 | Supplied as bar and forgings in most cases |
| Rod, bar, wire | ASTM B164 | ASTM B865 |
| Seamless tube and pipe | ASTM B165 | Available to order |
| Fasteners | ASTM F467, F468 | ASTM F467, F468 |
Frequently Asked Questions
Q: Is Monel K500 a stronger version of Monel 400?
A: Yes. K500 is the 400 composition modified with 2.30 - 3.15 % aluminium and 0.35 - 0.85 % titanium and precipitation hardened by ageing, giving roughly twice the tensile strength and three times the yield strength.
Q: Does K500 have the same corrosion resistance as 400?
A: In most media the two grades behave alike, including seawater and hydrofluoric acid. K500 is superior where erosion and impingement are present because of its higher hardness, but is slightly less resistant in some reducing acid environments.
Q: Can Monel 400 be heat treated to increase strength?
A: No. The 400 grade hardens only by cold working. Any attempt at thermal hardening will simply anneal the material and reduce its strength.
Q: Which grade is used for pump shafts?
A: K500. The high yield strength and hardness are needed to carry the shaft loads and resist wear at the bearings and seal areas while retaining seawater corrosion resistance.
Q: Are both grades magnetic?
A: Both are essentially non-magnetic at room temperature and retain low permeability at cryogenic temperature, with K500 showing a marginally higher permeability than the 400 grade.
Q: What happens if a K500 component is welded?
A: The weld and heat-affected zone lose the aged properties. Where full strength is required, the assembly must be re-solution treated and aged after welding, which is often impractical for large parts.