Alloy 400 and the well-known trade name for the same material refer to a single nickel-copper alloy. The registered designation is UNS N04400, and its European equivalent is NiCu30Fe, material number 2.4360. So the answer to the question is yes: the trade name and Alloy 400 describe the same 63% nickel, 30% copper composition. What differs is only the labelling convention. Buyers who specify by UNS number, by ASTM specification or by the older commercial name are ordering the same mill product.

That matters in practice because purchase documents, mill certificates and drawings may use different labels. A purchase order written against UNS N04400, ASME SB-165 or EN 2.4360 will deliver the same alloy, and any of those identifiers is acceptable as long as the mechanical and chemical requirements of the governing specification are met.

Chemistry and Governing Specifications

Element Requirement Typical function
Nickel 63.0% minimum Corrosion resistance, austenitic stability
Copper 28.0-34.0% Strength in seawater, resistance to reducing acids
Iron 2.5% maximum Solid solution strengthening
Manganese 2.0% maximum Desoxidation, workability
Carbon 0.30% maximum Controlled for ductility

Plate and sheet: ASTM B127, ASME SB-127

Seamless tube: ASTM B163, ASME SB-163

Seamless pipe: ASTM B165, ASME SB-165

Rod and bar: ASTM B164, ASME SB-164

Forgings and fittings: ASTM B564 and ASTM B366

European designations: NiCu30Fe, 2.4360, with the older DIN 17743 and 17753 coverage for wrought products

Mechanical and Physical Properties

Property Typical value
Density 8.80 g/cm3
Melting range 1300-1350 C
Tensile strength, annealed 480-550 MPa
Yield strength, 0.2% offset 195-240 MPa
Elongation, annealed 35-40%
Hardness, annealed About 120-150 HBW

The alloy keeps useful strength and ductility at sub-zero temperatures, which is why it is used for liquefied gas and cryogenic piping down to about -196 C. It is not a high-temperature material in the sense of a superalloy: continuous service in pressure applications is normally limited to about 480 C, and above that range strength falls away quickly. A common error in circulated data sheets is to quote a permissible service temperature of 1000 C by confusing the melting range with the working range. The correct engineering limit is about 480 C.

Corrosion Behaviour

Seawater and chloride service: excellent resistance to seawater and brine at moderate velocities, and virtually immune to chloride stress corrosion cracking, which makes it a standard choice for marine pump shafts, propeller shafts and condenser tubing.

Hydrofluoric and sulphuric acid: one of the few metallic materials accepted in hydrofluoric acid handling and in sulphuric acid service at moderate concentration and temperature, especially where the acid is deaerated.

Limitations: it is attacked by strongly oxidising media such as nitric acid and by aerated ammonia solutions, where it suffers stress corrosion cracking. Mercury contact must be avoided.

Typical Industrial Applications

Heat exchangers, condensers and boiler feedwater heaters

Propeller shafts, pump shafts and seawater pump components

Alloy 400 is produced in tube, pipe, sheet, plate, strip, round bar, hexagon bar, forgings, fittings, flanges and wire. Selection follows the corrosive medium first and the mechanical duty second: the alloy is normally specified where a copper-base material would corrode too quickly and a fully austenitic stainless steel would crack in chlorides, and where the higher cost of a nickel-molybdenum grade is not justified. Because the hardness of the annealed product is low, wear surfaces usually need hardfacing or a different material.

Frequently Asked Questions

Q: Is Alloy 400 the same as the nickel-copper alloy sold under a commercial trade name?
Yes. They are the same material: approximately 63% nickel with 28-34% copper, registered as UNS N04400 and standardised in Europe as NiCu30Fe, 2.4360.

Q: What is the maximum service temperature of Alloy 400?
About 480 C for continuous service in pressure equipment. Quoting 1000 C is incorrect, because that figure comes from the melting range rather than from the allowable working range.

Q: Is Alloy 400 suitable for hydrofluoric acid?
Yes, it is one of the standard metallic materials for hydrofluoric acid and for sulphuric acid at moderate concentration and temperature, and it is preferred where dissolved oxygen is kept low.

Q: Can Alloy 400 be welded?
Yes. It has good weldability by shielded metal arc, gas tungsten arc and gas metal arc processes. Matching nickel-copper filler is used, and the joint area should be clean and free of sulphur-bearing contamination.

Q: How does Alloy 400 behave in seawater?
It resists seawater and brine well at moderate flow velocity and is immune to chloride stress corrosion cracking, which is why marine shafting is a classic application. High velocity, erosion and galvanic coupling still need to be evaluated.