Jan 29, 2024 Leave a message

astm-b444-(1)-(1).pdf

Nickel Alloy UNS N06625: Composition, Mechanical Properties and Product Forms

Overview of Nickel Alloy UNS N06625

UNS N06625 is a non-magnetic, corrosion resistant and oxidation resistant nickel-chromium alloy. Its high strength comes from the hardening effect of molybdenum and niobium held in solid solution within the nickel-chromium matrix, not from precipitation treatment. The alloy resists a very wide range of severe corrosive environments, including high-temperature oxidation and carburisation, and it keeps useful strength and toughness from low temperature up to about 1093 °C.

Its resistance to pitting, crevice corrosion and chloride stress corrosion cracking, combined with high corrosion fatigue strength, makes it a standard material for seawater and marine hardware: springs, seals, bellows for diving controls, cable connectors, fasteners, flexures and oceanographic instrument components, in addition to aerospace applications.

Chemical Composition

Element Content, % Effect
Nickel, Ni 58.0 min Matrix, toughness, non-magnetic behaviour
Chromium, Cr 20.0–23.0 Oxidation and general corrosion resistance
Molybdenum, Mo 8.0–10.0 Pitting, crevice and reducing-media resistance
Niobium plus tantalum, Nb+Ta 3.15–4.15 Strength, stabilisation
Iron, Fe 5.0 max Matrix balance
Carbon, C 0.10 max Creep and ductility balance
Cobalt, Co 1.0 max Residual element
Manganese and silicon 0.50 max each Processing control
Phosphorus and sulphur 0.015 max each Cleanliness and hot workability

Chromium, molybdenum and niobium act together: chromium builds the passive film, molybdenum keeps that film stable in chloride media, and niobium restores strength after welding and elevated-temperature exposure.

Mechanical Properties of Coil and Wire Products

Property Requirement
Ultimate tensile strength 120 ksi min, equal to 827 MPa min
Yield strength, 0.2% offset 60 ksi min, equal to 414 MPa min
Elongation 30% min for sections over 0.040 in
Hardening route Cold work only; the alloy cannot be hardened by heat treatment
Weldability Excellent welding and brazing behaviour with matching or base-metal filler

Because there is no hardening heat treatment, the delivered temper and the amount of cold reduction define the final strength. Coil supplied in the annealed temper develops the values above as minimums, and further cold reduction raises strength at the cost of elongation.

Physical Properties and Thermal Expansion

Property Value
Mean coefficient of thermal expansion, 20–204 °C 7.3 × 10−6 in/in/°F, equal to 13.1 µm/m/°C
Mean coefficient of thermal expansion, 20–315 °C 7.5 × 10−6 in/in/°F, equal to 13.5 µm/m/°C
Mean coefficient of thermal expansion, 20–427 °C 7.7 × 10−6 in/in/°F, equal to 13.9 µm/m/°C
Magnetic permeability, annealed, H = 200 Oe 1.0006
Modulus of elasticity in tension 30.2 × 10&sup6; psi, about 208 GPa

The low and predictable expansion values let the alloy be used with austenitic stainless steel and other nickel grades in mixed assemblies without excessive thermal stress, while the near-unity permeability suits instrument and sensor components.

Product Forms and Surface Finishes

Strip, foil and ribbon supplied as hot rolled, annealed and descaled, or cold rolled, annealed and descaled.

Round, flat, square and special-shaped wire for springs, mesh, connectors and electrode applications.

No. 1 finish: hot rolled, annealed and descaled, for applications where a smooth surface is not required.

2D finish: cold rolled, annealed and descaled, matte surface for deep-drawn parts and where lubricant must be retained.

2B and bright annealed finishes: a light polished-roll pass produces a smooth surface for visible or lightly formed parts.

Polished grades in specified grit sizes, extra clean bright annealed material, and wire with grease or soap coating as a forming lubricant.

Coil dimensions, temper and finish are agreed against the forming operation, since the finish controls friction and lubricant retention during deep drawing and the temper controls springback in wire forming.

Frequently Asked Questions

Q: Can UNS N06625 be hardened by heat treatment?
No. The alloy cannot be hardened by thermal treatment; strength is developed by cold working, and annealing is used to restore ductility.

Q: What tensile and yield values apply to coil product?
Ultimate tensile strength of 120 ksi, or 827 MPa, minimum, with 0.2% offset yield strength of 60 ksi, or 414 MPa, minimum.

Q: Why is the alloy suited to seawater service?
It resists pitting, crevice corrosion and chloride stress corrosion cracking and offers high corrosion fatigue strength, which suits fasteners, springs and marine instrument parts.

Q: Is the alloy magnetic?
No. Annealed material has a magnetic permeability of about 1.0006 at 200 Oe, so it behaves as a non-magnetic material.

Q: What expansion behaviour should be allowed for in design?
Mean expansion rises from about 13.1 to 13.9 µm/m/°C between 20 °C and 427 °C, which is moderate for a nickel alloy and close to austenitic stainless steel.

Q: Which finishes are available?
Hot rolled annealed and descaled, 2D matte, 2B, bright annealed, polished, extra clean bright annealed, and wire with grease or soap coating for forming.

Send Inquiry

whatsapp

Phone

E-mail

Inquiry